鐵水預處理中錳和磷的氧化

The Oxidation of Manganese and Phosphorus in Hot Metal Pretreatment

  • 摘要: 采用石灰系熔劑處理低硅、高錳,中磷鐵水,以研究錳和磷的氧化。實驗結果表明:在1573~1623K,鐵水中﹝%Mn﹞>0.32時,錳比磷優先發生氧化;當﹝%Mn﹞<0.32時,磷比錳優先發生氧化。為了能順利地進行脫磷,必須將鐵水中的錳脫除到0.3%以下。通過熱力學計算,從理論上也證實了上述錳和磷的氧化規律。

     

    Abstract: The Oxidized relation between Mn and P in pretreatment of hot metal containing low Si, high Mn and mid P by using lime-based flux was investigated. The results show that when﹝%Mn﹞ is above 0.32, Mn is more preferential oxidized than P, and when﹝%Mn﹞is low 0.32, the result is contrary to one above mentioned at 1573-1623K. The Mn content which is low 0.3% in hot metal is necessary in order to obtain the sufficient dephosphorization.

     

/

返回文章
返回
<span id="fpn9h"><noframes id="fpn9h"><span id="fpn9h"></span>
<span id="fpn9h"><noframes id="fpn9h">
<th id="fpn9h"></th>
<strike id="fpn9h"><noframes id="fpn9h"><strike id="fpn9h"></strike>
<th id="fpn9h"><noframes id="fpn9h">
<span id="fpn9h"><video id="fpn9h"></video></span>
<ruby id="fpn9h"></ruby>
<strike id="fpn9h"><noframes id="fpn9h"><span id="fpn9h"></span>
www.77susu.com